化学配方数据库
| 配方类型: | ADHESIVES |
| 配方说明: | Aluminum Foil to Fiber Glass |
| 配方组成: | "Nebony" 100/5.0 Zinc Oxide/4.0 Toluene/37.0 R-29 "Neville" Resin, 10/15.0 "Nevsolv" T/60.0 Flat Bark (Natural Rubber)/8.5 "Nevastain" B/0.1 |
| 配制方法: | The flat bark is banded on cool tight rolls (0.020 inch) and the zinc oxide and "{nevastain" B are added together. MIlling is continued for about ten minutes. The batch is removed from the mill, cut into small pieces, and dissolved in the toluene. The "Nebony" 100 and R-29 "Neville" Resin 10 are dissolved in the "Nevsolv T." The rubber solution and resin solution are then mixed together. |