化学配方数据库
| 配方类型: | ADHESIVES |
| 配方说明: | Glass Cloth Laminate (Wet Lay-Up) Adhesive |
| 配方组成: | Vinyl Toluene/38.00 Antioxidant/0.25 Trimethylol Propane Trimethacrylate/5.00 A-172 Vinyl Tris (2-Methoxyethoxy) Silane/0.60 "Ricon" 100/57.00 Type of Glass Reinforcement/181 type-heat cleaned Peroxide Catalyst/3.00 |
| 配制方法: | The reinforcing material-glass cloth-is impregnated with the resin formulation, press-cured for 30 minutes at 320F, and then post-cured for 3 hours at 350F. |
| 返回数据库查询 |