化学配方数据库
| 配方类型: | ADHESIVES |
| 配方说明: | Insulated Glass Sealant |
| 配方组成: | Toluene (dry)/20 Part GMF/- "Age-Rite" White/- "Cabosil" M5/5 PbO2 (VFC, 0.33\m)/7.5 GMF/3.5 "Silane" A-187/4 "Age-Rite" White/1.5 (Cont.) "Enjay" Butyl LM 430/75 "Enjay" Butyl LM 430/25 Toluene (dry)/20 "Cabosil" M5/- "Silane" A-187/- "OMYA" BLH/75 "OMYA" BLH/- PbO2 (VFC, 0.33\m)/- |
| 配制方法: | Characteristics Pot Life 2 hrs. Cures Overnight Toluene will cause a chemical dew point in an insulated glass Toluene will cause a chemical dew point in an insulated glass unit. This is avoided by using activated carbon, or large pore size Molecular Sieve and/or silica gel in the spacer. |
| 返回数据库查询 |