化学配方数据库
| 配方类型: | EMULSIONS & DISPERSIONS |
| 配方说明: | DBPC Dispersion |
| 配方组成: | Triethanolamine/2.0 Di-tert-butyl-paracresol/60.0 Potassium hydroxide/0.5 Stearic Acid/6.0 Water/96.0 |
| 配制方法: | Dissolve the stearic acid and triethanolamine in 80 parts of water at 70C with gentle stirring; then dissolve the potassium hydroxide. Next add slowly with stirring di-tert-butyl-para-cresol, which is just above its melting point (70C) and stir until the mixture is homogeneous. Allow it to cool to 40C while stirring, and add 16 parts of cool water. |