化学配方数据库
| 配方类型: | EMULSIONS |
| 配方说明: | "Castorwax" Emulsion |
| 配方组成: | Stearic acid/2.14 Water/85.56 Triethanolamine/1.07 "Castorwax"/10.70 "Triton" X-100/0.53 |
| 配制方法: | Melt the "Castorwax" and stearic acid together and bring to a temperature of about 212F. At the same time add the triethanolamine and "Triton" X-100 to about one third of the total water and bring to its boiling point. Add the melted "Castorwax"-acid mix slow to the TEA water solution with rapid agitation. While the temperature is still above 200[F, run the emulsion through a colloid mill several times to ensure a small particle size. The remaining water at about 200F can then be added to the emulsion in the colloid mill. Cool the mixture slowly to room temperature with continued agitation. |