配方类型: METALS
配方说明: Recovery of Zinc from Dross (U.S. Patent 2,701,194)
配方组成: Sodium Chloride/21
Barium Chloride/31
Fuse and ad
Calcium Fluoride/3
Calcium Chloride/48
配制方法: This flux melts at 850F and can be heated to 1300F without fuming.
From 10 to 20% of this flux is stirred into the dross and rabbled until the oxides separate from the metal.