| 配方类型: | COATINGS |
| 配方说明: | Wall Paper Coating |
| 配方组成: | "Purina Protein"/100 Borax/15 Sodium Sulfite/1 Water, 180-200F./75 Water (ambient)/208 Ammonium Hydroxide, 26 Be/2 Water, 180-200F./2 |
| 配制方法: | Add 208 parts water to steam-jacketed mixing tank equipped with paddle agitator. The paddle width should be slightly less than the diameter of the tank. Start agitation and heat to 200-105F. Add 100 parts Purina Protein and mix 30 min. Add 1 part sodium sulfite dissolved in 2 parts water at 180-200F. Note: Some mixing tanks have line valves set apart from agitation-if so, draw off this unmixed portion and pour into tank. Repeat throughout process. Add 15 parts borax dissolved in 75 parts water at 180-200F. and mix 30 min. Add 2 parts ammonium hydroxide. Adjust dispersion to desired solids with water and mix 10 min. At this point a bactericide such as Dowicide G is dissolved in a quantity of hot water. The quantity of dry preservative is generally 0.5-1.0% on the total weight of the dispersion. A pine oil emulsion is normally added for defoaming, as a preservative, and as a leveling agent. Pine oil is added on the basis of 0.1-0.5% of the total volume of the coating mix. The emulsion helps to prevent oil sp |
| 返回数据库查询 |