返回 化工助手
化学配方数据库
配方类型: PAPER
配方说明: Lithographic Paper (Coating (Glossy)
配方组成: Alkaline dispersion of Casein/100
d: Polymer Emulsion:
Polyvinyl Acetate Emulsion, 36% solids, plasticized/10
Place in suitable vessel and blow with live steam for approximately
35 minutes or until an even, white dispersion results. Or, boil with 1
part morpholine added, using agitation
"Duroxon" J-324/3
Tap Water/15
a: Wax Dispersion:
b: Pigmentation:
Kaolin, Paper-Coating Quality/150
c: Binder:
(25% solids)
配制方法: Mix all ingredients in a roller mill for approximately 25 minutes.
Pass the mixture through a screen-type filter to eliminate gross impurities. Then process the mixture through an ordinary colloid mill.
this coating is directly applied to the paper from a trough. It is then air-dried and, lastly, calendered by friction.