化学配方数据库
| 配方类型: | COATINGS |
| 配方说明: | Black Oxide Electrodeposition Primer |
| 配方组成: | XP-2042 (75% NV)/55.0 Pounds triethylamine/6.5 Amino resin (90% NV)/10.0 Black iron oxide/25.0 Pounds Water (deionized)/760.0 |
| 配制方法: | Electrodeposition Conditions: 1. pH---8 to 8.5. 2. Voltage---50 to 100 volts. 3. Peak amps---4-6 amps. 4. Time---30 to 60 seconds. 5. Bake schedule---5 minutes at 350f or 20 minutes at 300F. 6. Dry film---0.5 to 1.0 mil. 7. XP-2042 is the replenishment vehicle. |