化学配方数据库
| 配方类型: | POLISH |
| 配方说明: | Liquid Solvent Floor Polish |
| 配方组成: | Stoddard Solvent/89 "Petrolite" P-25 Paraffin Wax, 140 AMP/7-6 "Petrolite" P-20/4-6 Formula No. "Petrolite" P020 "Petrolite" P-25/4-5 Paraffin Wax, 140 AMP/7-6 Stoddard Solvent/89 |
| 配制方法: | Heat solvent to 180F and add molten waxes. Cool with stirring and pour into containers between 100F and 140F. Caution: do not stir rapidly when mixture approaches pouring temperatures. Rapid agitation will adversely affect the formation of crystals and may cause separation of solvent. P-20 and P-25 have excellent solvent-binding properties and if the polish is compounded properly, there should be less than 5% of free solvent. P-20 and P-25 have very similar properties, but P-25 is recommended when a viscous gel is desired. The formulas given contain 11% solids and have a good cleaning action during application. The finished wax film is free from tack and buffs readily to a high gloss. The hardness of the film can be regulated by varying the ratio of synthetic wax to paraffin. |
| 返回数据库查询 |