| 配方类型: | POLISH |
| 配方说明: | Emulsion of "Shanco" W-1119 Wax/Polyethylene |
| 配方组成: | Morpholine/20 Polyethylene (Emulsifiable)/80 Water---(208-212F)/610 Oleic Acid (Pale)/20 (Solids 16%)/750 lb "Shanco" W-1119 Wax/20 lb |
| 配制方法: | Heat the "Shanco" W-1119 Wax, polyethylene and oleic Acid to a fluid melt at 250F. Add the morpholine and mix slowly for about 5 minutes. Remove open flames before adding the morpholine. Adjust temperature of the base at around 240F. Have the water at 208-210F, just under boiling and agitate rapidly to produce a vortex. Pour the hot base slowly into the side of the vortex at a rate that will not create boiling. Mix rapidly for 5 minutes. Cool while agitating slowly. |