| 配方类型: | POLISH |
| 配方说明: | Scuff-Resistant Floor Polish |
| 配方组成: | "RWL"-201 latex (40%)/50.0 Formalin/1.5 "A-C" polyethylene 629 emulsion (15%)/160.0 Water/412.0 Tributoxyethyl phosphate/6.0 "RWL"-112 latex (40%)/198.0 "Igepal" CO-630/3.0 "Shanco 1165-S resin solution (15%)/180.0 Diethylene glycol/4.0 |
| 配制方法: | Add the water to the polishing mixing kettle. Then add the "RWL"-201 latex with stirring. Adjust pH to 8.0 to 9.0 with 28% ammonium hydroxide. Then add the "RWL"-112 latex, the resin solution, and the polyethylene emulsion with stirring. Combine the plasticizers and add slowly with adequate agitation to the latex-resin-wax mixture. Stir for 1/2 hr. Then add the formalin and adjust the final pH to 8.8 to 9.0 with 28% ammonium hydroxide. |