配方类型: TEXTILES AND THEIR TREATMENT
配方说明: Pressure Dyeing Polyesters
配方组成: Dyeing temperature
配制方法: The above concentrations generally give optimum results. For very heavy shades with hard-to -build dyes, or light shades with hard-to-level dyes, increased amounts may be needed.
Set bath at 100-120F with 1-2% MSP. Add required amount of "Tanavol" APP. Run 5 minutes. Add disperse dyes properly pasted with diluted "DS-14". Adjust pH to 6 with acetic acid. Heat at 2-3f/minute to dyeing temperature (225-260F). Run about 1 hour. Dye adds, if necessary, may be made at 180F. When on shade, cool and rinse well.