配方类型: COATINGS
配方说明: Vinyl Alkyd Coating
配方组成: "Solvesso" 150/25
Formula No.
"Exon" XR-6337/75
TCP/5
"Paraplex" G-62 or Equivalent/5
"Thermolite" RS-20; Mark KCB/2.5
DIDP/10
"Thermolite" RS-20; Mark KCB/2.5
"Solvesso" 150/50
DIBK/15
TCP/5
"Amberlac" 292G/150
"Amberlac" 292G/150
"Exon" XR-6337/75
"Paraplex" G-62 or Equivalent/5
DIBK/30
Isopropanol/10
Isopropanol/20
DIDP/10
配制方法: Disperse "Exon" XR-6337 in plasticizers, DIBK, heat stabilizer and Isopropanol. Charge to a ball mill and grind to an N.S. of 7-8. (It may be necessary to dilute with a small amount of "Solvesso" 150.) Add "Amberlac" 292G and remaining "Solvesso" 150.
Formulation B will probably give a lower viscosity with "Exon" XR-6337 during grinding than Formulation A and also have less tendency to gel.
Remove at desired N.S. grind.
Bake Schedule: 15 minutes at 180C. on DT 36 Panels.